Laserfiche WebLink
J <br />21 <br />E <br />E <br />i <br />le 10 z 10' 10' 10' 10" IU <br />TIME ihoursl <br />Figure 6. Stress Rupture Line for .4--dsymmetric Loading of a?EGeomembrane. <br />Derived with -Elevated Temperature <br />• and Bonaparte,s• <br />20 <br />TEMPERATURE- Zr C <br />)5 • AIL .• ••R a4, <br />�e <br />E _ �� ♦ate <br />CP <br />10 1P • 2 <br />it <br />¢ . � • p• ♦ A 0.] ►•OURS <br />0 22 "OURS <br />us <br />Id ♦ o I • SSS HOURS <br />Z3.16 <br />W ♦ 23M FlOtJf1S <br />7� <br />• 77D0 HgURS <br />3.4 N /m M 1- 1.9 1 17300 ►�pt1R5 <br />So vEARS (PREDICTED) <br />0 <br />0 1.0 1.8 ) 5 10 t5 <br />(l <br />2.91 STRAIN (y ) <br />Figure 7. 50 -Year Isochronous Curve for Axisymmetric Loading of a PE Geomembrane, <br />Derived with Elevated Temperature Testing (after Berg and Bonaparte, 1993) <br />1452 - Vancouver. Canada - Geosynd=&s'93 <br />