Laserfiche WebLink
The standard kit mclu�the following materials and tools: - If you're not sure how fast it will set up, it is better to mix <br /> ,�,.y• - - - "" several small batches rather than one big one. <br /> d. Application <br /> BOX A Using the paint brush provided. DAB the resin mixture into the <br /> cloth rather than painting it on.You are trying to completely soak the <br /> 4 each I Qt.bottles PLASTEEL resin matting with resin,not just cover it. <br /> BOX B <br /> I each I Qt.bottle Resin emulsifier or Acetone <br /> 4 each 1 Oz.bottles CatalystowlZo <br /> �,/.l. f <br /> 6 each Star Mats <br /> 10 each Ma[strips e. Pipe and Risers <br /> For standard threaded fittings:Apply resin to the base of the pipe <br /> 6 each Plug mats and lop of tank and push down the matting circle as shown. <br /> -3 each 4"FlatPeP B PI plugs Impregnate with resin. <br /> Impregnate the strips of matting and wrap like tape around the <br /> 2 each Paint stirring sticks joint starting at the base and working upward. Apply any leftover <br /> 2 each 1-1/2"Paint brushes resin to the outside of the joints when done wrapping. <br /> 3 each Mixing cups For special bolt-up flanges: Apply generous coating of resin to <br /> exposed metal edges of flange and wrap with resin impregnated <br /> I each Sheet 60 grit sandpaper matting strips.Apply leftover resin to nuts and bolts. <br /> 4 each Hook Mats <br /> Additional material is supplied when tank configured with <br /> containment collars,special fittings,manholes or extension spools. ( ' <br /> h Preparation <br /> Do not mix the catalyst with the resin until all the pieces you wish It <br /> to impregnate have been fitted in place and the I"strips of matting 1l <br /> are laid out next to their corresponding pipe connections. Once the <br /> resin and catalyst are mixed,a chemical reaction begins that cannot <br /> be reversed.Working time for a mixed batch is about 30 minutes at f. Steel Plugs <br /> 700 E Higher temperatures make it set up more quickly,shortening Ager fitting fiberglass matting,lift it up and apply mixed resin to <br /> working time. For example,at 1000 F. you will have approximately the top of the tank surface when, the matting will contact. Stick <br /> 15 minutes of working time. The key things to remember are: matting over plug into wet resin and totally impregnate matting with <br /> (1) Be prepared and have all parts prefitted and in place before resin,dabbing in with paint brush as described above. <br /> mixing the resin. (2) Mix only as much resin as you can use in <br /> 30 minutes and mix it thoroughly - stir for at least I minute. fy Manhole,Extension Spool and Handling Hooks <br /> (3)Work quickly and efficiently. Lower temperatures increase resin Apply generous coating of resin impregnated matting strips to <br /> set-up time and require additional catalyst. exposed metal edges and to handling.hooks(matting precut).Apply <br /> leftover resin to nuts and bolts except on access cover. <br /> c. Mixing the catalyst <br /> Resin and catalyst must be mixed in the proper proportions so h. Cleanup <br /> that the resin will harden properly. Below is a list of some various Hands and tools may be cleaned with Resin Emulsifier before <br /> size batches you could mix. the resin has hardened. No solvent will work once the resin has <br /> hardened. <br /> RESIN CATALYST NOTE: <br /> The PLASTEEL' tank installation is not complete until all <br /> I qt. .... . . . .. . . . . . . . . . . . .. . . . . ..I/2 oz. exposed steel surfaces on tank are sealed with[he PLASTEEL° <br /> I pint .. . . . . . . . . . .. . . . . . . . . .. . . . .1/4 oz. fiberglass resin. <br /> I cup .. . . . . .. . . . . . . . . . . . . . . . . . . .1/8 oz. For additional assistance or information, call your <br /> PLASTEEL tank factory below: <br /> l <br /> Authorized PLASTEELa COMPOSIT tank manufacturers <br /> INSTALL WESZOW INDUSTRIA ACERO HALL TANK CO. DOOR MFG k6 TSTEEL METAL PRODUCTS TANX INC. SHINNNONINCUSTRY TANCUESGUMEX TECNOECOARGENTWA <br /> ftz a ..NIa n Obnn.EcuaOor N.6Ma Nock AR EswMick,CA Tam Fab.b su•anee.GA Cann onl NH Seel.Karca Torreon.`Aeam Buenos Aker."no, <br /> 15 011 9 459 211 (7601745-0971 Jain M25M (710)945.8393 1607)543-1272 <br /> CUUSmIASCORREAGUA .61PANSTEELWORKS Far(501)94S1477 Fa(760)746-9515 Faa12091733-rM Faa(770)932-5671 Fv(6031543-1270 TECNOECO CHILE TVG <br /> Panama.Panama Toa)a.Japan Sannaso.Club Tab.Hun9nN <br /> rnm a4ST4.97e <br />